[1]花能斌,黄旭方,黄杏芳.利用废陶瓷辊棒制备堇青石陶瓷材料[J].福建工程学院学报,2016,14(03):237-243.[doi:10.3969/j.issn.1672-4348.2016.03.007]
 Hua Nengbin,Huang Xufang,Huang Xingfang.Preparation of cordierite ceramics using ceramic roller waste[J].Journal of FuJian University of Technology,2016,14(03):237-243.[doi:10.3969/j.issn.1672-4348.2016.03.007]
点击复制

利用废陶瓷辊棒制备堇青石陶瓷材料()
分享到:

《福建工程学院学报》[ISSN:2097-3853/CN:35-1351/Z]

卷:
第14卷
期数:
2016年03期
页码:
237-243
栏目:
出版日期:
2016-06-25

文章信息/Info

Title:
Preparation of cordierite ceramics using ceramic roller waste
作者:
花能斌黄旭方黄杏芳
福建工程学院材料科学与工程学院
Author(s):
Hua Nengbin Huang Xufang Huang Xingfang
College of Materials Science and Engineering, Fujian University of Technology
关键词:
堇青石 废陶瓷辊棒 晶相 力学性能 显微结构
Keywords:
cordieriteceramic roller wastecrystalline phasemechanical propertymicrostructure
分类号:
TB31
DOI:
10.3969/j.issn.1672-4348.2016.03.007
文献标志码:
A
摘要:
利用废陶瓷辊棒作为主要原料采用高温煅烧法制备堇青石陶瓷材料,研究了烧成工艺对堇青石材料的晶相、显微结构和性能的影响。利用X射线衍射仪表征试样的晶相结构;利用扫描电子显微镜观察试样的显微结构;利用排水法测试试样的显气孔率和体积密度;通过万能试验机检测试样的抗弯强度。研究结果表明:试样经煅烧后形成堇青石陶瓷材料,主晶相为堇青石相,次晶相为镁铝尖晶石相。堇青石呈粒状分布,试样中具有一定量的玻璃相,均匀地分布着微米级的微孔。随着煅烧温度和保温时间的增加,显气孔率先减小后增大,体积密度先增大后减小,抗弯强度先增大后减小,最佳烧结工艺为煅烧温度1 350℃保温时间3h时,显气孔率最小为21 %,体积密度为1.96 g/cm3,抗弯强度最大为58 MPa。
Abstract:
In this study, cordierite ceramics was prepared by high temperature sintering using ceramic roller waste as raw materials. The effects of sintering process on the crystalline phases, microstructure and properties of cordierite samples were investigated. X-ray diffraction was carried out to characterize the crystalline structure of samples. The microstructure morphology of the sintered samples was observed by a scanning electron microscope. The apparent porosity and bulk density of the samples were measured using Archimedes’s method. Mechanical testing machine was employed to evaluate the bending strength of the specimen. The results show that the primary crystalline phase of cordierite ceramics obtained by sintering is cordierite, whereas the secondary crystalline phase of which is spinel. The cordierite crystals are in granular shape and bonded by glassy phase with micro-pores being uniformly distributed in the samples. As the sintering temperature and maintaining time increase, the apparent porosity of the samples first decreases and then increases, and the bulk density and bending strength of the samples first decrease and then increase. The optimal sintering properties are obtained at a sintering temperature of 1350℃ maintained for 3 h with an apparent porosity of 21 %, a bulk density of 1.96 g/cm3 and the maximum bending strength of 58 MPa.

参考文献/References:

[1] 汪潇,杨留栓,刘冉,等.堇青石陶瓷的研究现状[J].耐火材料,2009,38(3):297-299.
[2] 赵月明,郭从盛,谭宏斌.堇青石陶瓷的应用与制备进展[J].中国陶瓷,2011,47(10):7-9.
[3] 朱展鹏,姚远.影响堇青石合成的因素分析[J].陶瓷,2013,45(3):45-47.
[4] Zhou J,Dong Y,Hampshir S,el al.Utilization of sepiolite in the synthesis of porous cordierite ceramics[J].Applied Clay Science,2011,2(3):328-332.
[5] 李恒,杜庆洋,李国昌,等.淀粉固化法制备堇青石多孔陶瓷[J].人工晶体学报,2013,42(9):1036-1039.
[6] 彭超.利用累托石合成堇青石的研究[J].武汉理工大学学报,2004,8(2):1-64.
[7] 王琦,黄朝晖,欧阳欣,等.用粉煤灰和菱镁矿低温制备堇青石质多孔材料[J].硅酸盐学报,2012,4(5):745-750.
[8] 郭伟,陆洪彬,冯春霞,等.以稻壳为硅源和成孔剂合成多孔堇青石陶瓷的研究[J].硅酸盐通报,2011,30(2):431-434.
[9] 胡婉莹,延锦丽,吕峰.辊道窑陶瓷辊棒的化学矿物组成与性能研究[J].现代技术陶瓷,2007,111(1):20-23.
[10] 李远兵,黄凯,吴清顺,等.陶瓷辊棒的研究现状[J].中国陶瓷,2009,45(6):3-7.
[11] 花能斌,苏丽凤,黄旭方,等.利用废陶瓷辊棒制备多孔轻质莫来石材料[J].福建工程学院学报,2014,12(1):9-12.
[12] 方斌正.煅烧铝矾土合成堇青石及其在太阳能储热材料中的应用研究[D].武汉:武汉理工大学,2013.
[13] 于岩.铝型材厂工业污泥综合利用的基础研究[D].福州:福州大学,2006.